Trothwy Crynodiad Atalydd ar gyfer Atal Tyllu mewn Alcali Crynodol
For 316L stainless steel sheathed electric heating tubes in 50% sodium hydroxide (NaOH) at 150°C-such as in caustic evaporator heaters or chemical concentrators-chloride ions (500 ppm) cause rapid pitting unless inhibited by sulfate (SO₄²⁻). The sulfate-to-chloride weight ratio (R = SO₄²⁻/Cl⁻) determines pitting resistance. Below R = 3:1, pitting initiates within 500-1,000 hours. At R = 3:1 to 5:1, pitting is delayed to 1,000-3,000 hours. At R >5:1, pitting is suppressed for >5,000 o oriau. Y gymhareb gritigol ar gyfer cychwyn tyllu 1,000-awr ar 500 ppm Cl⁻ yw tua R=2.5:1 i 3:1. Mae'r erthygl hon yn meintioli'r union drothwy cymhareb sylffad i glorid ar gyfer tyllu o fewn 1,000 o oriau o dan yr amodau ymosodol hyn.
Mecanwaith Atal Sylffad mewn-Tymheredd Uchel costig
Ar 150 gradd mewn 50% NaOH, mae'r ffilm goddefol ar 316L yn gromiwm ocsid/hydrocsid cyfoethog. Mae ïonau clorid yn tarfu ar y ffilm trwy ffurfio-cymhlethau cloro hydawdd. Mae ïonau sylffad yn cystadlu â chlorid am safleoedd arsugniad. Ar y gymhareb gritigol, mae gorchudd sylffad yn atal digon o arsugniad clorid ar gyfer cychwyn pwll. Mae'r ataliad yn dilyn isotherm Langmuir cystadleuol.
Sylffad Meintiol-Cymhareb Clorid yn erbyn Amser Cychwyn Pitting
Mae profion rheoledig o 316L mewn 50% NaOH ar 150 gradd gyda 500 ppm Cl⁻ a chrynodiadau sylffad amrywiol (fel Na₂SO₄) wedi sefydlu'r amseroedd cychwyn tyllu canlynol.
| SO₄²⁻: Cymhareb Cl⁻ (wt/wt) | Sylffad (ppm) | Amser cychwyn tyllu (oriau) | Cyfradd pitsio (mm/blwyddyn) | Amser i Dyllu (wal 1.5 mm, misoedd) | Argymhellir ar gyfer Gwasanaeth 1,000+ Awr |
|---|---|---|---|---|---|
| <1:1 | <500 | <100 | >0.50 | <2 | Nac ydw |
| 1:1 | 500 | 150-250 | 0.40-0.60 | 2-4 | Nac ydw |
| 1.5:1 | 750 | 250-400 | 0.30-0.50 | 3-5 | Nac ydw |
| 2:1 | 1,000 | 400-700 | 0.20-0.40 | 4-6 | Ymylol |
| 2.5:1 | 1,250 | 700-1,200 | 0.10-0.25 | 6-10 | Derbyniol (ffiniol) |
| 3:1 | 1,500 | 1,200-2,000 | 0.05-0.15 | 10-20 | Oes |
| 4:1 | 2,000 | 2,000-3,500 | 0.03-0.08 | 15-30 | Oes |
| 5:1 | 2,500 | >5,000 | <0.02 | >75 | Oes |
| >5:1 | >2,500 | >5,000 | <0.02 | >75 | Oes |
Casgliad:Mae angen cymhareb sylffad-i-clorid Yn fwy na neu'n hafal i 3:1 (1,500 ppm SO₄²⁻ ar 500 ppm Cl⁻) i ohirio cychwyn tyllu y tu hwnt i 1,000 awr mewn 50% NaOH ar 150 gradd . Yn R=2.5:1, mae tyllu'n digwydd o fewn 700-1,200 awr, ffiniol ar gyfer gwasanaeth 1,000 awr.